(6)  Make sure that the area to be repaired is clean and free from any contaminants.  If necessary, use acetone and re-sand the area. 
(7)  Apply two layers of anti-static spray filler to the repair area.  Obey the filler manufacturer's instructions. 
(8)  Allow the anti-static filler to dry.  At 20 to 25 °C (68 to 77 °F), 60 to 75 % relative humidity. 
(9)  Carefully sand the anti-static filler with 320 grit sanding paper.  Remove as little anti-static filler as possible. Do not sand through the edges. 
(10)  Make sure that the area to be repaired is clean and free from any contaminants.  If necessary, use acetone and re-sand the area. 

Doc # 6.02.01 Page 211
Rev. 4 09 Jan 2003

51-20-00
Structures
AMM

Detail Steps/Work Items  Key Items/References 
(11)  Apply the coating paint.  Obey the paint manufacturer's instructions. 
(12)  Allow the coating paint to dry.  90 minutes at 45 °C (113 °F), then 2 days at 20 °C (68 °F). 

C. Painting a Small Repair Area
This procedure must be followed when the diameter of the area which must be painted is 200 mm (8 inches) or less.
Detail Steps/Work Items  Key Items/References 
WARNING: DO NOT GET ACETONE, FILLER, OR PAINT ON YOUR SKIN. ACETONE, FILLER, AND PAINT CAN CAUSE SKIN DISEASE. WARNING: DO NOT BREATHE ACETONE, FILLER, OR PAINT FUMES. ACETONE, FILLER, AND PAINT FUMES CAN CAUSE DISEASE. CAUTION: THERE MUST BE NO GREASE OR DUST ON THE REPAIR AREA. GREASE AND DUST PREVENT A GOOD BOND. 
(1)  Make sure that the area to be repaired is clean and free from any contaminants.  If necessary, use acetone and re-sand the area. 
(2)  Apply 2 layers of HS filler to the repair area.  Obey the filler manufacturer's instructions. 
(3)  Allow the HS filler to cure.  2 hours at 45 °C (113 °F). 
(4)  Lightly sand the HS filler with 320 grit sanding paper. 
(5)  Make sure that the area to be repaired is clean and free from any contaminants.  If necessary, use acetone and re-sand the area. 
(7)  Apply the coating paint.  Obey the paint manufacturer's instructions. 
(8)  Allow the coating paint to dry.  90 minutes at 45 °C (113 °F), then 2 days at 20 °C (68 °F). 

Page 212 Doc # 6.02.01 09 Jan 2003 Rev. 4
51-20-00
AMM
Structures

9. Repairs
A. Class 4 Repairs
The repair of minor scratches, abrasions or similar damage which is not a crack or a puncture in the skin.
Detail Steps/Work Items  Key Items/References 
WARNING: DO NOT GET ACETONE ON YOUR SKIN. ACETONE CAN CAUSE SKIN DISEASE. WARNING: DO NOT BREATHE ACETONE FUMES. ACETONE FUMES CAN CAUSE DISEASE. 
(1)  Sand the repair area with 150 grit sanding paper. 
(2)  Make sure that the area to be repaired is clean and free from any contaminants.  If necessary, use acetone. 
(3)  Apply putty to the repair area to fill any damage.  Obey the putty manufacturer's instructions. Fill to the original contour of the structure. 
(4)  Allow the putty to cure.  5 to 20 minutes. 
(5)  Lightly sand the putty with 150 grit sanding paper. 
(6)  Apply filler(s) and paint coat.  Refer to Paragraph 8 in this Section. 

Doc # 6.02.01 Page 213
Rev. 4 09 Jan 2003

51-20-00
Structures
AMM

Table 2 - Material Specifications
WLB No. (German Aviation Standard)  Manufacturer and Type  Material  Weave  Weight per unit area [g/m2]  Thick-ness [mm]  Scarf [mm] 
8.4548.60  Interglas 92110  glass  2/2 twill  163  0.17  7 
 